112 年 國立臺灣大學材料科學與工程研究所碩士班甲組《材料科學》
第 1 題12 分
- True or False (reason your answer if you think the statement is false) (12%):
(a) Graphite is soft because of the weak sp² C-C bond strength. (2%)
(b) It is possible to manufacture a single crystal without dislocations or vacancies at room temperature. (2%)
(c) Let represents the angle between the normal to the slip plane of a BCC crystal and the applied stress direction, and represents the angle between the slip and stress directions. Typically, . (2%)
(d) Because the two-phase coexisting state in the Cu-Ni binary system under given pressure at 1 atm appears as a "field" in the binary phase diagram, the "number of degrees of freedom" is 2. (2%)
(e) Using and , equations, the true stress () and strain () may be transferred from engineering stress () and strain (). Those equations are invalid beyond the necking point, though. (2%)
(f) Because engineering fatigue data are impractical to collect from normal laboratory tests, we need to employ the Larson-Miller parameter to conduct data extrapolation. (2%)
登入後即可作答並保存紀錄。
核心觀念:
本題涵蓋材料科學六大核心領域:(a) 碳同素異形體之混成軌域與層間鍵結、(b) 點缺陷(空孔)與線缺陷(差排)的熱力學平衡性質、(c) 單晶滑移幾何與施密特定律(Schmid's law)、(d) 定壓二元相圖之吉布斯相律(Gibbs phase rule)、(e) 真實應力-應變與工程應力-應變之體積守恆轉換條件,以及 (f) 高溫潛變外推參數(Larson-Miller parameter)與疲勞試驗之區別。
逐題判斷與理由解析:
(a) False(錯誤)
- 理由: 石墨(graphite)為層狀六方晶格結構,同一平面層內的碳原子採 混成軌域,彼此以極強的 共價鍵與非定域 鍵結合(鍵能高達約 ,比鑽石的 單鍵更強)。石墨之所以質軟且具潤滑性,是因為層與層之間僅靠微弱的凡得瓦力(van der Waals forces,次級鍵)結合,在外力剪切下層面極易發生相對滑動,而非因為 共價鍵強度弱。
(b) False(錯誤)
- 理由:
- 空孔(Vacancies)為熱力學平衡點缺陷: 空孔的引入會大幅增加晶體的構型熵(configurational entropy, ),使系統的吉布斯自由能降低()。因此在任何高於絕對零度(,包含室溫)的熱平衡狀態下,晶體必然存在有限的平衡空孔濃度 ,不可能在室溫下製備出完全沒有空孔的單晶。
- 差排(Dislocations)為非平衡線缺陷: 差排的形成能極高且構型熵貢獻極小,並非熱力學平衡缺陷。透過特殊晶體成長技術(如柴氏法 Czochralski 或浮區法 Floating-zone 生長半導體級矽單晶,或製備微米級單晶晶鬚 whiskers),確實可以在室溫下獲得無差排(dislocation-free)的單晶,但仍必然含有熱平衡空孔。因此「在室溫下同時無差排且無空孔」的敘述為錯誤(若指可製備無差排但含平衡空孔之單晶,亦說明二者不可混為一談)。
(c) True(正確)
- 理由: 根據施密特定律(Schmid's law),分解剪應力為 ,其中滑移面法線向量 與滑移方向向量 因為滑移方向必位於滑移面內,故兩向量互相垂直(,夾角為 )。
在三維空間中,外加應力軸單位向量 與兩正交單位向量 、 的方向餘弦滿足: 其中 為應力軸與 軸之夾角。由此可知: 對銳角 而言,必滿足: 其中等號 僅在外加應力軸 恰好完全落在由滑移面法線 與滑移方向 所張成的平面內(即 )時才成立;對一般任意晶體取向(),恆有 。故此敘述正確。
(d) False(錯誤)
- 理由: 在定壓( 固定)條件下,凝聚態吉布斯相律(Condensed Gibbs Phase Rule)為:
對 二元系統(成分數 )的 兩相共存區(相數 ),其熱力學自由度(number of degrees of freedom)為 (單變系,univariant),而非 。
雖然 兩相區在二元溫度-整體組成()相圖上呈現為一個二維「區域(field)」,但決定各相熱力學狀態的強度變數是溫度 與各相平衡組成 、(而非合金整體組成 ):一旦在該兩相區內指定了溫度 (僅 個獨立自由度),固相組成 與液相組成 即由固相線與液相線完全唯一確定;
第 2 題11 分
- The concentration of substitutional solute atoms in solids (11%):
(a) A researcher, Guang-En, wants to calculate the density of a hypothetical A-4.4wt.%B alloy. The information Guang-En has obtained is listed as follows:- A and B atomic masses are 26.981 amu and 63.456 amu, respectively.
- B atoms present in the form of random substitutional solute in A matrix forming an FCC lattice.
- The lattice parameter of this FCC crystal is a function of B atomic percentage and temperature: . Here is the atomic percentage in unit "at.%B," and is the temperature in unit "°C."
Based on the information provided, calculate the mass density of A-4.4wt.%B at 540°C. (4%)
(b) Now, Guang-En wants to diffuse Z atoms into an X wafer using predeposition and drive-in heat treatments. The X wafer initially has a background concentration of Z atoms atoms/m³. In the first, or predeposition step, impurity Z atoms are diffused into the X wafer, and the surface composition of the Z, , also remains constant over time atoms/m³. The suggested predeposition treatment time, , is 10 minutes. We may approximate the total surface concentration of Z impurities in the X solid that was introduced during the predeposition treatment, , as:
where represents the diffusion coefficient of Z atoms in X solid during predeposition, and the unit of should be atoms/m². The second "drive-in diffusion" treatment is used to transport Z atoms farther into the X wafer in order to provide a more suitable concentration distribution without increasing the overall impurity content. This treatment is carried out at a higher temperature, 1200°C, in an oxidizing atmosphere to form an oxide layer on the surface. The diffusion of Z atoms through this XO₂ layer is slow, so very few Z atoms diffuse out of and escape from the X wafer. After "drive-in diffusion," the junction depth, , representing the x-position where the diffusing Z concentration is just equal to , can be approximated as:
where and are "the diffusion coefficient of Z atoms in X solid" and "time period," respectively, during "drive-in diffusion" treatment. If Guang-En wants to achieve μm after two hours of "drive-in diffusion" treatment, what predeposition temperature should he use? For the diffusion of Z in X, the preexponential factor and diffusion activation energy are m²/s and 3.65 eV/atom, respectively. (7%)
登入後即可作答並保存紀錄。
(a)A–4.4 wt.%B 合金密度
核心觀念
FCC 晶胞每個單位晶胞含有 4 個原子。合金密度可由「晶胞質量 ÷ 晶胞體積」求得:
其中 是每莫耳合金原子的平均質量, 是亞佛加厥常數, 是晶格常數。
解題方法
先將重量百分比換算為原子百分比。假設合金總質量為 100 g,則
因此 B 的原子分率為
故 at.%B。代入晶格常數公式,並以題目指定的攝氏溫度計算:
平均原子量為
將晶格常數換成公分, cm,代入 FCC 密度公式:
(b)預沉積溫度
核心觀念
預沉積階段的表面濃度固定,總摻雜量由預沉積的擴散係數與時間決定;驅入階段則近似為固定總劑量的擴散。兩階段的擴散係數皆遵循 Arrhenius 關係:
題目給定的活化能是 eV/atom,因此使用 eV/K,且 Arrhenius 式中的溫度必須使用 K。
解題方法
先求 1200°C 驅入時的擴散係數。 K:
將結深公式取指數並整理,可得預沉積帶入的總劑量:
使用 s、 m 及 atoms/m³:
由預沉積劑量公式解出 :
第 3 題6 分
- Crystallization kinetics of a fluxing agent (6%):
A fluxing agent initially in its liquid form crystallizes at a temperature below the melting point of this fluxing agent; the fraction of crystallization, X, as a function of the crystallization time, t, and the isothermal holding temperature, , may be represented as the "extended" Avrami equation shown in the following:
where is the preexponential factor, is the activation energy of crystallization, R is the gas constant, is the incubation time, and n is the Avrami exponent associated with the nucleation and growth mechanism. Explain how we can vary , , and conduct linear regression to obtain constants , , , and n. (6%)
登入後即可作答並保存紀錄。
核心觀念
這是延伸型 Avrami(JMAK)方程式,包含兩層關係:
- 在固定溫度下,結晶分率 與時間 的關係可經雙重取對數變成直線。
- 速率常數隨溫度符合 Arrhenius 關係,取對數後對 也是直線。
先定義與溫度有關的速率常數:
原式寫成:
解題方法
步驟一:線性化
取一次自然對數後乘以負號:
再取一次自然對數:
步驟二:固定 、改變 (第一次線性迴歸,求 、、)
- 在數個不同的恆定溫度 (皆低於熔點)下做等溫結晶實驗,量測每個溫度下 隨 的變化(例如以 DSC 放熱量或 XRD 結晶量換算)。
- 孕育時間 :可由 開始大於 0 的起始時間估計,再微調;也可在合理範圍內掃描 ,選擇使迴歸直線決定係數 最大者。
- 每個溫度下,以 為橫軸、 為縱軸作迴歸:
- 斜率 ,即 Avrami 指數。
- 截距 ,因此 。注意截距含有因子 ,必須先除以 。
步驟三:改變溫度 (第二次線性迴歸,求 、)
由 的定義取對數:
以 ( 為絕對溫度 K)為橫軸、步驟二求得的 為縱軸作迴歸:
第 4 題11 分
- The research and development in titanium alloys (11%):
(a) A pure titanium originally at 1066°C would transform from BCC βTi to HCP αTi at 883°C. However, if adding β-stabilizing elements such as vanadium, an appreciable amount of βTi phases can be retained at room temperature. Nowadays, Ti-6Al-4V (wt.%) has been the most widely used titanium alloy where αTi and βTi coexist. One of the typical heat treatments is the slow furnace cooling the solution-treated Ti-6Al-4V from 1066°C (~50°C above βTi→αTi transformation temperature). While conducting X-ray diffraction (XRD) analysis with a wavelength of 1.54Å on the cooled specimen, there are peaks at 2θ=35°, 39°, 40°, 41°, 54°, 58°, 64°, 72°, and 75° in the XRD pattern. By understanding (i) 2θ=35° corresponds to plane of HCP αTi with c/a ratio 1.582, and (ii) 2θ=40° corresponds to plane of BCC βTi, index the remaining peaks. (5%)
Note 1: the interplanar spacing formula for hexagonal crystals is:
Note 2: the rule of missing reflection for HCP crystal is:
and is odd ( is an integer)
(b) Determine the critical crack length for a through crack within a thick plate of a Ti-6Al-4V alloy with an equiaxed grain structure that is under uniaxial tension. The fracture toughness is 66 MPa√m and its fracture stress is 910MPa. Assume in the fracture toughness equation. (3%)
(c) Another typical heat treatment for Ti-6Al-4V alloy is water quenching from 1066°C. This heat treatment is expected to let Ti-6Al-4V form a structure consisting of all "titanium martensite," plate-like HCP, and its lattice parameters are slightly different from HCP αTi. However, "titanium martensite" is relatively soft compared to iron-carbon martensite in steel. Explain why "titanium martensite" is softer by first listing three important strengthening mechanisms of "iron-carbon martensite" and then indicating one of those mechanisms is nearly absent in "titanium martensite." (3%)
登入後即可作答並保存紀錄。
(a) X 光繞射峰指認
核心觀念
利用布拉格定律將繞射角換算為晶面間距,再以晶體結構的晶面間距公式比對晶面指數:
對六方晶系:
對體心立方晶系:
以下峰位視為取整後的實測值;合金成分與量測誤差會使峰位和理想計算值略有差異。
解題方法
已知 是 HCP αTi 的 峰,故 。由布拉格定律:
對此晶面,,因此:
以這組晶格常數代入六方晶系公式,可得到 αTi 各晶面的預期間距,再與待指認峰位比對。題目所給的 HCP 消光規則也可用來排除不允許的反射。
同理,已知 對應 BCC βTi 的 峰:
以 BCC 晶面間距公式比對其餘峰,可辨認 與 峰。
| 晶相 | 晶面指數 | 判定依據 | |
|---|---|---|---|
| αTi,HCP | HCP 的 峰預期約在 | ||
| αTi,HCP | 預期約在 附近 | ||
| αTi,HCP | 預期約在 附近 | ||
| βTi,BCC | BCC 中 ,預期約 | ||
| αTi,HCP | 預期約在 附近 | ||
| βTi,BCC | BCC 中 ,預期約 | ||
| αTi,HCP | 預期約在 附近 |
解題技巧:先用已知峰反推出晶格常數,再分類比對其他峰,通常比逐一猜測晶面指數更有效。BCC 晶面還須符合 為偶數的條件;HCP 晶面則須檢查題目給定的消光規則。
(b) 臨界裂縫長度
核心觀念與推導
厚板中的穿透裂縫可用下式描述:
其中 是裂縫半長。題目給定 ,整理得:
第 5 題10 分
- The polished section of one sintered CeO2 specimen is shown below. The specimen was sintered at 1500°C for 1 h. The grain boundaries were revealed by thermal etching at 1400°C for 0.5 h. (10%)
(i) What is roughly the relative density of the specimen?
(ii) What is roughly the size of the CeO2 grains?
登入後即可作答並保存紀錄。
這題主要考驗學生對陶瓷燒結、顯微結構觀察(相對密度、晶粒尺寸)的理解。
(i) 相對密度估計
核心觀念: 燒結後的陶瓷試樣,其密度與理論密度之比稱為相對密度。從顯微照片中,可以通過觀察晶界、孔隙等來估計相對密度。
觀察顯微照片:
照片顯示了燒結後的 CeO2 試樣的顯微結構。可以看到明顯的晶粒和晶界。
- 孔隙 (Pores): 燒結過程中,孔隙是影響密度的主要因素。孔隙可能存在於晶粒內部或晶界上。
- 晶界 (Grain Boundaries): 晶粒之間的界面。
- 晶粒 (Grains): 獨立的晶體區域。
估計方法:
- 目測法: 觀察照片中孔隙所佔的面積比例。如果孔隙佔據的面積比例很小,則相對密度很高。
- 比例尺: 照片下方有一個比例尺,標示了 1 µm。這可以幫助我們估計晶粒尺寸和孔隙的大小。
分析照片:
照片中,晶粒界線清晰,大部分區域被晶粒覆蓋。雖然可以看到一些孔隙(尤其是在晶界上),但總體來看,孔隙的總體積佔比較小。
- 如果孔隙佔據了 10% 的體積,則相對密度約為 90%。
- 如果孔隙佔據了 5% 的體積,則相對密度約為 95%。
- 如果孔隙佔據了 20% 的體積,則相對密度約為 80%。
從圖上看,孔隙的體積佔比似乎不大。大多數晶粒界線都很清晰,沒有看到大量的開口孔隙。相對密度應該比較高。
假設孔隙佔總體積的 5-10%。
因此,相對密度約為 90-95%。
更精確的估計(如果可能):
在沒有其他資訊的情況下,目測是最直接的方法。
照片顯示,燒結溫度為 1500°C,時間為 1 小時。這個條件對於氧化物陶瓷(如 CeO2)來說,通常可以達到較高的燒結密度。
如果孔隙主要集中在晶界,並且尺寸不大,那麼整體密度會比較高。
觀察照片,孔隙似乎沒有佔據太大的比例。
結論:
基於目測,孔隙的總體積比例估計在 5% 到 10% 之間。
因此,相對密度約為 90% - 95%。
(ii) CeO2 晶粒尺寸估計
核心觀念: 晶粒尺寸是指單個晶粒的平均尺寸。從顯微照片中,可以使用比例尺來估計晶粒尺寸。
第 6 題10 分
- The iron ions in Wustite (iron oxide) can exist in both Fe2+ and Fe3+ states. In order to maintain the electroneutrality, the chemical formula for Wustite is often represented as FexO. (10%)
(i) Please choose from (a) x<1.0 or (b) x=1.0 or (c) x>1.0, which one is correct.
(ii) Please explain briefly.
登入後即可作答並保存紀錄。
這題考驗學生對化學計量、氧化物結構以及電荷平衡的理解。
核心觀念: 氧化物的化學式代表了其中陽離子和陰離子的比例。為了保持整體電荷的中性,陽離子和陰離子的總正電荷必須等於總負電荷。
分析:
Wustite (FeO) 是一種鐵的氧化物,其中鐵離子可以以 Fe 和 Fe 的形式存在。氧離子通常帶有 -2 的電荷 (O)。
化學式為 FeO,意味著每 1 個氧原子,有 個鐵原子。
總電荷必須為零:
由於鐵離子可以是 Fe 和 Fe 的混合物,因此平均鐵離子電荷必須介於 +2 和 +3 之間。
設 Fe 的比例為 ,Fe 的比例為 。則 。
平均鐵離子電荷 。
由於 ,所以 。
平均鐵離子電荷 。
因為 (比例),所以平均鐵離子電荷的範圍是:
當 (全是 Fe) 時,平均電荷 。
當 (全是 Fe) 時,平均電荷 。
所以,平均鐵離子電荷介於 +2 和 +3 之間。
將平均鐵離子電荷代入電荷平衡方程:
因為平均鐵離子電荷介於 +2 和 +3 之間 ():
- 當平均鐵離子電荷為 +2 時,。這對應於 FeO(純 Fe)。
- 當平均鐵離子電荷為 +3 時,。這對應於 FeO(純 Fe)。
- 當平均鐵離子電荷介於 +2 和 +3 之間時, 的值介於 和 之間。
即 。
然而,Wustite 的化學式通常表示為 FeO,且其組成範圍為 FeO 到 FeO。這意味著 的值小於 1。
為什麼會這樣呢?
這是因為在 Wustite 的結構中,存在結構缺陷,即鐵離子空位。
例如,FeO 可以看作是 Fe 和 Fe 的混合物,並且存在鐵離子空位。
假設化學式為 FeO。
如果鐵離子只有 Fe,那麼化學式應為 FeO ()。
但由於存在 Fe,為了維持電荷平衡,需要減少陽離子總數,或者說,需要留下一些陽離子空位。
例如,考慮 FeO。
假設有 1 個 O,則總負電荷為 -2。
總正電荷必須為 +2。
假設鐵離子有 Fe 和 Fe。
在 FeO 中,平均每 0.95 個鐵原子帶 +2 的總電荷。
平均每個鐵原子的電荷 。
這表示存在 Fe 和 Fe 的混合物。
設 Fe 的摩爾分數為 ,Fe 的摩爾分數為 。
總鐵原子數為 。
。
。
。
。
。
所以,在 FeO 中,約 89.5% 的鐵是 Fe,10.5% 的鐵是 Fe。
這種情況下,鐵離子的平均電荷是 +2.105。
第 7 題10 分
- Draw the repeat units of the polymers formed from the following monomers: (2 pts x 5 = 10 pts):
(a) HOOH + H₂CO----OCH₃
(b) H₂N------NH₂ + Cl----Cl
(c) HO----OH + Cl----Cl
(d) O=C----O
(e) H₃CO----O
登入後即可作答並保存紀錄。
核心觀念
本題考查聚合反應中「單體結構如何轉換成聚合物重複單元」:
- 碳碳雙鍵 開鍵,形成加成聚合物。
- 二胺與二醯氯縮合,形成聚醯胺,副產物為 。
- 二醇與二醯氯縮合,形成聚酯,副產物為 。
- 繪製重複單元時,必須保留單體的主鏈原子與側基,並以方括號及 表示聚合鏈。
題目文字中的部分長鍵與原子標示已遺失;以下依可辨識的標準結構解答。可辨識部分為:
- :過氧化氫,引發劑。
- :甲基乙烯基醚。
- :己二胺。
- :己二醯氯。
- :乙二醇。
解題方法
判斷重複單元時,先找出單體的反應官能基:
- :雙鍵開鍵,形成 主鏈。
- 與 :形成 醯胺鍵。
- 與 :形成 酯鍵。
每個重複單元的兩端,必須能與相鄰單元繼續連接。
(a) 過氧化氫與甲基乙烯基醚
甲基乙烯基醚為:
過氧化氫 是引發劑,不會成為聚合物的重複單元。碳碳雙鍵開鍵後,原本的 轉變為單鍵,形成:
因此聚合物為聚甲基乙烯基醚:
(b) 己二胺與己二醯氯
反應單體為:
以及:
胺基與醯氯基縮合:
反覆縮合後,重複單元為:
這是尼龍 6,6 類型的聚醯胺結構。聚合物主鏈中的特徵鍵為醯胺鍵:
(c) 乙二醇與己二醯氯
反應單體為:
以及:
羥基與醯氯基縮合:
因此形成聚酯,重複單元為:
聚合物主鏈中的特徵鍵為酯鍵:
(d)
題目目前可辨識的結構為二氧化碳:
二氧化碳本身沒有能夠在一般加成聚合中直接連接成高分子鏈的雙鍵或雙官能基,因此單獨以 作為單體時,不能直接畫出一般線型聚合物的重複單元。
第 8 題10 分
- Sketch the chemical structure of SBS copolymer (5 pts). Why is it a thermoplastic elastomer? (5 pts)
登入後即可作答並保存紀錄。
核心觀念:
-
SBS 三嵌段共聚物(ABA Triblock Copolymer):
SBS 為 Styrene-Butadiene-Styrene(苯乙烯-丁二烯-苯乙烯)三嵌段共聚物,由兩端為聚苯乙烯(Polystyrene, PS)硬鏈段(hard segments)與中間為聚丁二烯(Polybutadiene, PB)軟鏈段(soft segment)以共價鍵連接而成。 -
熱塑性彈性體(Thermoplastic Elastomer, TPE)的微相分離與物理交聯原理:
傳統硫化橡膠依賴不可逆的化學共價交聯(如硫橋鍵),一旦交聯即無法再加熱熔融加工(屬熱固性彈性體);而 SBS 則是利用兩嵌段熱力學不相容所產生的微相分離(microphase separation)與兩種鏈段玻璃轉移溫度()的巨大差異,在室溫下形成可逆的物理交聯網路(reversible physical crosslinks)。
解題方法:
一、SBS 共聚物之化學結構式(Chemical Structure of SBS Copolymer)
SBS 由兩端的聚苯乙烯嵌段(重複單元:)與中間的 1,4-聚丁二烯嵌段(重複單元:)組成:
[ Polystyrene (PS) ] [ Polybutadiene (PB) ] [ Polystyrene (PS) ]
(Hard Segment) (Soft Segment) (Hard Segment)
H H H H H H H H
| | | | | | | |
---[ C - C ]----------------[ C - C = C - C ]----------[ C - C ]---
| | n | | m | | n
H C6H5 H H H C6H5
(苯環) (苯環)
以化學示性式表示為:
二、為何 SBS 為熱塑性彈性體?(Why SBS is a Thermoplastic Elastomer)
SBS 能同時具備「室溫下的橡膠高彈性(elastomeric behavior)」與「高溫下的熱塑加工性(thermoplastic processability)」,歸因於以下三個微觀機制:
-
熱力學不相容性與微相分離(Microphase Separation):
聚苯乙烯(PS)嵌段與聚丁二烯(PB)嵌段在熱力學上互不相溶(正的混合焓 ),但由於兩者以共價鍵連接在同一條高分子鏈上,無法發生巨觀相分離,因此會自組裝形成奈米尺度的微相分離結構:少量的 PS 鏈段聚集形成分散的球狀或柱狀剛性微區(PS domains),均勻散佈在連續的 PB 軟相基地(PB matrix)中。 -
室溫下()表現出橡膠彈性:
- 軟鏈段(PB 嵌段,): 室溫高於聚丁二烯的玻璃轉移溫度(),因此連續相 PB 鏈段處於高活動性的橡膠態(rubbery state),分子鏈柔順且容易在外力下拉伸構型展開,提供高彈性變形與熵彈性回復力。
- 硬鏈段(PS 嵌段,): 室溫低於聚苯乙烯的玻璃轉移溫度(),因此兩端的 PS 微區處於剛性固態的玻璃態(glassy state)。
第 9 題10 分
- What are low dielectric constant (low-K) materials and high dielectric constant (high-K) materials used in silicon-based semiconductor techniques? Why low-K and high-K materials are essential for advanced CMOS technologies? (10%)
登入後即可作答並保存紀錄。
核心觀念
相對介電常數 (亦寫 或 )表示材料在電場下被極化、儲存電能的能力。平行板電容為
其中 為面積、 為介電層厚度。傳統矽基 CMOS 以二氧化矽(,)作絕緣層。元件微縮後,電晶體閘極(前段製程,FEOL)與金屬內連線(後段製程,BEOL)對 的需求相反:閘極要大電容,導線之間要小電容。因此分別發展 High- 與 Low- 材料。
解題方法
一、Low-κ 材料(用於內連線)
- 定義與應用: 低於 ()的絕緣材料,用作後段金屬導線之間與各層之間的層間介電層(ILD/IMD)。
- 常見材料:摻氟氧化矽(FSG, 約 3.5);摻碳氧化矽(SiOC:H,又稱 CDO 或 OSG, 約 2.7–3.0);有機高分子介電材料;多孔性介電材料(以奈米孔洞降低密度, 可更低)以及氣隙結構。降低 的方法是引入極化率較低的化學鍵,並加入孔洞(空氣 )。
- 為何必要:微縮使導線截面縮小、電阻 升高,導線間距縮小、寄生電容 升高,內連線的延遲成為限制晶片速度的主因。使用 Low- 介電層因 ,可以:
- 降低 延遲,提高訊號速度;
- 降低導線充放電的動態功耗();
- 降低相鄰導線的耦合電容,減少串音(crosstalk)。
- 挑戰:Low- 材料(尤其多孔材料)機械強度較低、易吸水,製程整合(研磨、蝕刻)較難。
二、High-κ 材料(用於閘極介電層)
- 定義與應用: 顯著高於 的絕緣氧化物,用作 MOSFET 的閘極介電層(亦用於 DRAM 電容介電層)。
- 常見材料:鉿基氧化物如 ( 約 20–25)、,另有 、、 等;過渡期曾使用氮氧化矽。
- 為何必要:MOSFET 的驅動電流與單位面積閘極電容 成正比,要維持閘極對通道的控制並抑制短通道效應, 必須維持夠大。若只靠把 變薄來增加 ,薄到約 1–2 nm 以下時,電子會直接穿隧通過閘極氧化層,閘極漏電流急劇增加,造成靜態功耗過大。改用 High- 材料可以在較大的物理厚度下取得同樣的電容,穿隧漏電流因此大幅降低。
- 等效氧化層厚度(EOT):
第 10 題10 分
- Please describe the relationships among permittivity, electric dipole momentum, polarization vector, electric susceptibility, and complex refractive index. What is the dispersion behavior of permittivity with frequency? (10%)
登入後即可作答並保存紀錄。
核心觀念
這題問五個量的關係,從微觀到巨觀,再延伸到光頻與頻散:電偶極矩 (微觀)→ 極化向量 (單位體積偶極矩)→ 電極化率 ( 對 的比例)→ 介電常數 ( 與 的比例)→ 複數折射率 (光波傳播,)。
解題方法
- 電偶極矩
正負電荷 、相距 的偶極:
原子或分子在局部電場 下產生的誘發偶極矩為 ( 為極化度 polarizability)。具永久偶極的分子(如水),其偶極也會受電場影響而部分排向。
- 極化向量
單位體積內的偶極矩總和:
單位 , 為偶極子數密度。
- 電極化率
線性、各向同性介電質中:
無因次,表示材料被電場極化的難易程度。
- 介電常數
電位移:
因此
- 複數折射率
交變電場下,極化會有相位落後與損耗, 為頻率的複數函數。以 的時間慣例,
實部 代表儲能,虛部 代表損耗。非磁性介質()由馬克士威方程式得 。令 ( 為折射率,決定相速度 ; 為消光係數,決定振幅衰減):
所以
透明區 ,簡化為 。(有些教科書用 慣例,會寫成 、,結果相同,只要全文慣例一致即可。)
介電常數隨頻率的頻散行為
總極化由四種機制貢獻,每一種都有自己能跟上電場的頻率上限,隨頻率升高,慣性大的機制依序「跟不上」而退出:
- 空間電荷(界面)極化:晶界、相界、電極界面的電荷堆積,只在很低頻(約 kHz 以下)有貢獻。
- 偶極(取向)極化:永久偶極分子轉向,是弛豫(Debye)型:頻率接近 時, 下降, 出現損耗峰。範圍約在無線電波至微波。